# Shrinkage cavity (ISO 6520-1 ref. 202): causes and detection

Source: https://www.therness.com/defects/202-shrinkage-cavity/
Language: en

ISO 6520-1 group 2 · Cavities

ISO 6520-1 reference 202 is a cavity formed by volumetric contraction on solidification, not by trapped gas. Cause matrix, why radiography reads the two differently, and where acceptance is set.

ISO 6520-1 reference

202

Group

2 — Cavities

Also called

Shrinkage cavity, Shrinkage void, Solidification shrinkage

A shrinkage cavity forms for a completely different reason than the gas pores that dominate ISO 6520-1 group 2: it is a volumetric-contraction problem, not a trapped-gas problem. As molten metal solidifies it shrinks, and if not enough liquid feeds the last region to freeze, a void opens where the feed path sealed off first. Reference 202 is the parent designation for that mechanism, the way [2011](https://www.therness.com/defects/2011-porosity/) is the parent designation for the single gas pore.

Because the cause is feeding, not shielding, the cause matrix looks nothing like the porosity family’s: deposition rate and travel speed through the end of a run, joint geometry that traps a feed path, and — in additive work — a layer transition that does not remelt or feed the previous layer the way a single continuous pass would. [Crater pipe](https://www.therness.com/defects/2024-crater-pipe/), reference 2024, is the specific case of this at the weld termination itself, the same location a [crater crack](https://www.therness.com/defects/104-crater-crack/) forms at, for a related reason.

The practical distinction for an inspector is the radiograph’s edge shape, not its presence: a smooth round trace is gas, an irregular or dendritic-edged one is shrinkage, and the two get graded and controlled through entirely different levers.

## Typical causes

What produces shrinkage cavity, the mechanism, and the control that removes it

| Cause | Mechanism | Control |
| --- | --- | --- |
| Insufficient filler metal to compensate for solidification contraction | Metal shrinks as it freezes; without enough liquid feeding the last region to solidify, a void opens where the feed path closed off first. | Maintain deposition rate and travel speed inside the qualified window through the last part of a run. |
| A feed path that freezes shut before the last liquid solidifies | In a heavy section or a poorly designed joint, the solidification front can seal the last liquid pocket off from further feed, guaranteeing a void. | Treat a joint geometry that repeatedly produces the same void location as a design issue, not a parameter issue. |
| An interrupted or unfed layer transition in additive deposition | Stopping a layer without adequate remelt or feed into the previous one leaves the same unfed-last-liquid condition between layers. | Qualify layer-to-layer transition technique the same way a single-pass procedure is qualified. |

## Detection: which route finds it

The column that matters most is the last one. An inspection family marked as not finding this imperfection will not find it however carefully it is applied, and planning around that is cheaper than discovering it during a final examination.

Detection routes for shrinkage cavity, and what each one can and cannot see

| Family | Method | Capability | What it sees |
| --- | --- | --- | --- |
| Visual | Visual testing to ISO 17637 | Does not find it | The cavity forms below the last solidified surface and leaves no surface indication unless it happens to intersect the final layer or bead. |
| Thermal | In-process infrared thermography | Limited | Solidification shrinkage is a volumetric effect, not a thermal event distinct from ordinary cooling; the thermal signature does not separate it from a sound weld. |
| Camera | High-speed weld pool imaging | Does not find it | The void opens as the metal finishes freezing, after the pool the camera observes has already gone solid. |
| NDT | Radiographic testing to ISO 17636 | Primary route | A radiograph reads a shrinkage cavity as an irregular, often feathered or dendritic-edged indication, distinct from the smooth round trace of a gas pore. |

## Where acceptance is defined

Therness pages never reproduce a standard's acceptance values: those tables are copyrighted and belong in the copy you hold. What follows is the pointer — which document governs, and which part of it to open.

Documents that set the acceptance criteria, and the clause topic to read

| Standard | Clause topic | Note |
| --- | --- | --- |
| ISO 5817 | Quality levels for imperfections in steel, nickel and titanium joints, indexed by ISO 6520-1 reference number | Assessed on its own terms, separately from gas porosity in the same group. Read it in the standard. |
| ASME BPVC Section VIII | Radiographic acceptance for pressure vessels, with examination methods in Section V | Acceptance lives in the construction code, not in the qualification code. |

## Standards that govern this imperfection

- [ISO 5817](https://www.therness.com/standards/iso-5817/)Does ISO 5817 govern your joint? Scope decision flow for the steel, nickel and titanium quality-level standard, the codes it is read with, and the records that evidence conformity.

## Imperfections found alongside it

- [Crater pipe (ref. 2024)](https://www.therness.com/defects/2024-crater-pipe/)Cavities — ISO 6520-1 group 2.
- [Gas pore (ref. 2011)](https://www.therness.com/defects/2011-porosity/)Cavities — ISO 6520-1 group 2.
- [Crater crack (ref. 104)](https://www.therness.com/defects/104-crater-crack/)Cracks — ISO 6520-1 group 1.

## Terms used on this page

[Heat input](https://www.therness.com/glossary/heat-input/)

Heat input is the energy delivered to a joint per unit length of weld, calculated from arc voltage, welding current and travel speed and multiplied by the thermal efficiency factor of the process.

[Weld pool](https://www.therness.com/glossary/weld-pool/)

The weld pool is the localized volume of molten metal created by the welding heat source, into which filler metal is added and from which the weld bead forms as it solidifies.

## Where this imperfection dominates

Additive manufacturing and near-net-shape production

### [Monitoring for wire arc additive manufacturing](https://www.therness.com/applications/wire-arc-additive-manufacturing/)

WAAM is welding with no interpass inspection access and no wrought equivalent to compare against. The codes that apply, the four monitoring pain points, and which Therness signal addresses each.

## Questions about shrinkage cavity

### Is a shrinkage cavity the same thing as porosity?

No. Porosity is trapped gas that could not escape the pool. A shrinkage cavity forms because not enough liquid metal fed the last region to solidify — a volumetric problem, not a gas problem — even though both sit in the same ISO 6520-1 cavities group.

### Can gas shielding fix a shrinkage cavity?

No. Shielding controls gas entrapment, which is a different mechanism. A shrinkage cavity is controlled through deposition rate, feed and joint design, not shielding.

### How does radiography tell a shrinkage cavity apart from a gas pore?

By edge shape. A gas pore reads as a smooth, rounded indication; a shrinkage cavity reads as irregular and often feathered or dendritic at the edge, reflecting the last liquid metal freezing around it.

## See the condition, not the consequence

Most weld imperfections are produced by conditions that exist while the arc is running. Therness records those conditions on every weld, so a suspect run is known on the shift that made it rather than in a batch report.