Discover HeatCore AI

ISO 6520-1 group 2 · Cavities

Crater pipe (ISO 6520-1 ref. 2024): causes and detection

ISO 6520-1 reference 2024 is a shrinkage cavity at the arc-stop point, from insufficient crater fill. Cause matrix, why it shares a location with crater cracking, and where acceptance is set.

ISO 6520-1 reference
2024
Group
2 — Cavities
Also called
Crater pipe, Crater shrinkage, End crater pipe

A crater pipe is a shrinkage cavity with a fixed address: the point where the arc was terminated. ISO 6520-1 reference 2024 names it as the crater-specific case of shrinkage cavity, reference 202 — same mechanism, insufficient feed for solidification contraction, but concentrated at a stop instead of occurring mid-run.

The stop is the highest-risk moment in a weld: breaking the arc removes the feed source at the same instant the crater still has to solidify and shrink. Without a crater-fill technique — a run-out tab, a progressive current taper, or a reverse pass over the crater — nothing compensates for that contraction, and a pipe opens.

The same stop point is also where crater cracking forms, for a related but distinct reason: shrinkage strain opens a hot crack rather than a cavity. The two can appear together or separately, so a crater found on inspection is worth reading carefully rather than assumed to be one or the other — the fix differs, and both trace back to a skipped crater-fill step.

Typical causes

What produces crater pipe, the mechanism, and the control that removes it
CauseMechanismControl
Arc broken without a crater-fill technique or run-out tabStopping current abruptly leaves the still-molten crater with no continued feed to compensate for the metal about to shrink as it freezes.Qualify and follow a crater-fill sequence — reducing current progressively or backing over the crater — rather than releasing the trigger.
A stop-start point with no reverse or overlap passWithout a short reversal into already-deposited metal, the crater freezes as an isolated pool with nothing left to feed its own contraction.Require a reverse or overlap distance at every planned stop, and treat every unplanned stop the same way.
High travel speed or low heat input right before the stopA thin, fast-frozen pool at the moment of arc break has less reservoir of liquid metal to feed the crater as it contracts.Hold parameters inside the qualified window through the last few centimetres of a run, not only through the body of it.

Detection: which route finds it

The column that matters most is the last one. An inspection family marked as not finding this imperfection will not find it however carefully it is applied, and planning around that is cheaper than discovering it during a final examination.

Detection routes for crater pipe, and what each one can and cannot see
FamilyMethodCapabilityWhat it sees
VisualVisual testing to ISO 17637Supporting signalA crater pipe often shows as a visible depression or pinhole at the stop, one of the few shrinkage cavities visual inspection actually catches.
ThermalIn-process infrared thermographyLimitedThe arc-break event is visible in the record, but the resulting void is a volumetric effect the thermal signature does not distinguish from a sound stop.
CameraHigh-speed weld pool imagingSupporting signalShows whether a crater-fill technique was actually executed, which is the condition that determines whether a pipe forms.
NDTRadiographic testing to ISO 17636, penetrant testing to ISO 3452-1 for a surface-breaking pipePrimary routeRadiography sizes a subsurface pipe; penetrant testing confirms one broken through at the stop.

Where acceptance is defined

Therness pages never reproduce a standard's acceptance values: those tables are copyrighted and belong in the copy you hold. What follows is the pointer — which document governs, and which part of it to open.

Documents that set the acceptance criteria, and the clause topic to read
StandardClause topicNote
ISO 5817Quality levels for imperfections in steel, nickel and titanium joints, indexed by ISO 6520-1 reference numberAssessed as a shrinkage cavity at the stop location, with its own extent basis distinct from a gas pore. Read it in the standard.
API 1104Acceptance for pipeline girth welds, treated separately from structural workEvery stop and restart on a girth weld is a crater-pipe candidate, so pipeline procedures give the tie-in its own scrutiny.

Questions about crater pipe

Does a crater pipe always come with a crater crack?

No, but they share the same weak point. A crater crack (104) is a hot crack from shrinkage strain at the stop; a crater pipe (2024) is a cavity from insufficient feed. Either can occur alone, and both are more likely where crater fill was skipped.

Is crater pipe unique to arc-stop points?

Yes — it is the crater-specific case of shrinkage cavity (202). A shrinkage void elsewhere, away from a stop-start, is graded as 202 instead.

Does running back over the crater fix the risk on the next weld too?

It fixes that stop, not the condition. If heat input right before the stop was already thin, the next stop carries the same risk regardless of technique at the crater.

See the condition, not the consequence

Most weld imperfections are produced by conditions that exist while the arc is running. Therness records those conditions on every weld, so a suspect run is known on the shift that made it rather than in a batch report.

Progetto cofinanziato nell'ambito del PR Piemonte FSE+ 2021-2027,