# Crater pipe (ISO 6520-1 ref. 2024): causes and detection

Source: https://www.therness.com/defects/2024-crater-pipe/
Language: en

ISO 6520-1 group 2 · Cavities

ISO 6520-1 reference 2024 is a shrinkage cavity at the arc-stop point, from insufficient crater fill. Cause matrix, why it shares a location with crater cracking, and where acceptance is set.

ISO 6520-1 reference

2024

Group

2 — Cavities

Also called

Crater pipe, Crater shrinkage, End crater pipe

A crater pipe is a shrinkage cavity with a fixed address: the point where the arc was terminated. ISO 6520-1 reference 2024 names it as the crater-specific case of [shrinkage cavity](https://www.therness.com/defects/202-shrinkage-cavity/), reference 202 — same mechanism, insufficient feed for solidification contraction, but concentrated at a stop instead of occurring mid-run.

The stop is the highest-risk moment in a weld: breaking the arc removes the feed source at the same instant the crater still has to solidify and shrink. Without a crater-fill technique — a run-out tab, a progressive current taper, or a reverse pass over the crater — nothing compensates for that contraction, and a pipe opens.

The same stop point is also where [crater cracking](https://www.therness.com/defects/104-crater-crack/) forms, for a related but distinct reason: shrinkage strain opens a hot crack rather than a cavity. The two can appear together or separately, so a crater found on inspection is worth reading carefully rather than assumed to be one or the other — the fix differs, and both trace back to a skipped crater-fill step.

## Typical causes

What produces crater pipe, the mechanism, and the control that removes it

| Cause | Mechanism | Control |
| --- | --- | --- |
| Arc broken without a crater-fill technique or run-out tab | Stopping current abruptly leaves the still-molten crater with no continued feed to compensate for the metal about to shrink as it freezes. | Qualify and follow a crater-fill sequence — reducing current progressively or backing over the crater — rather than releasing the trigger. |
| A stop-start point with no reverse or overlap pass | Without a short reversal into already-deposited metal, the crater freezes as an isolated pool with nothing left to feed its own contraction. | Require a reverse or overlap distance at every planned stop, and treat every unplanned stop the same way. |
| High travel speed or low heat input right before the stop | A thin, fast-frozen pool at the moment of arc break has less reservoir of liquid metal to feed the crater as it contracts. | Hold parameters inside the qualified window through the last few centimetres of a run, not only through the body of it. |

## Detection: which route finds it

The column that matters most is the last one. An inspection family marked as not finding this imperfection will not find it however carefully it is applied, and planning around that is cheaper than discovering it during a final examination.

Detection routes for crater pipe, and what each one can and cannot see

| Family | Method | Capability | What it sees |
| --- | --- | --- | --- |
| Visual | Visual testing to ISO 17637 | Supporting signal | A crater pipe often shows as a visible depression or pinhole at the stop, one of the few shrinkage cavities visual inspection actually catches. |
| Thermal | In-process infrared thermography | Limited | The arc-break event is visible in the record, but the resulting void is a volumetric effect the thermal signature does not distinguish from a sound stop. |
| Camera | High-speed weld pool imaging | Supporting signal | Shows whether a crater-fill technique was actually executed, which is the condition that determines whether a pipe forms. |
| NDT | Radiographic testing to ISO 17636, penetrant testing to ISO 3452-1 for a surface-breaking pipe | Primary route | Radiography sizes a subsurface pipe; penetrant testing confirms one broken through at the stop. |

## Where acceptance is defined

Therness pages never reproduce a standard's acceptance values: those tables are copyrighted and belong in the copy you hold. What follows is the pointer — which document governs, and which part of it to open.

Documents that set the acceptance criteria, and the clause topic to read

| Standard | Clause topic | Note |
| --- | --- | --- |
| ISO 5817 | Quality levels for imperfections in steel, nickel and titanium joints, indexed by ISO 6520-1 reference number | Assessed as a shrinkage cavity at the stop location, with its own extent basis distinct from a gas pore. Read it in the standard. |
| API 1104 | Acceptance for pipeline girth welds, treated separately from structural work | Every stop and restart on a girth weld is a crater-pipe candidate, so pipeline procedures give the tie-in its own scrutiny. |

## Standards that govern this imperfection

- [ISO 5817](https://www.therness.com/standards/iso-5817/)Does ISO 5817 govern your joint? Scope decision flow for the steel, nickel and titanium quality-level standard, the codes it is read with, and the records that evidence conformity.

## Imperfections found alongside it

- [Shrinkage cavity (ref. 202)](https://www.therness.com/defects/202-shrinkage-cavity/)Cavities — ISO 6520-1 group 2.
- [Crater crack (ref. 104)](https://www.therness.com/defects/104-crater-crack/)Cracks — ISO 6520-1 group 1.
- [Gas pore (ref. 2011)](https://www.therness.com/defects/2011-porosity/)Cavities — ISO 6520-1 group 2.

## Terms used on this page

[Heat input](https://www.therness.com/glossary/heat-input/)

Heat input is the energy delivered to a joint per unit length of weld, calculated from arc voltage, welding current and travel speed and multiplied by the thermal efficiency factor of the process.

[Weld pool](https://www.therness.com/glossary/weld-pool/)

The weld pool is the localized volume of molten metal created by the welding heat source, into which filler metal is added and from which the weld bead forms as it solidifies.

## Where this imperfection dominates

Pipeline construction — oil, gas and product transportation

### [Weld monitoring for pipeline construction](https://www.therness.com/applications/pipeline/)

Cross-country and plant piping welded under API 1104 and the ASME B31 transportation codes. The four monitoring pain points that cost pipeline contractors most, and which Therness signal addresses each.

## Questions about crater pipe

### Does a crater pipe always come with a crater crack?

No, but they share the same weak point. A crater crack (104) is a hot crack from shrinkage strain at the stop; a crater pipe (2024) is a cavity from insufficient feed. Either can occur alone, and both are more likely where crater fill was skipped.

### Is crater pipe unique to arc-stop points?

Yes — it is the crater-specific case of shrinkage cavity (202). A shrinkage void elsewhere, away from a stop-start, is graded as 202 instead.

### Does running back over the crater fix the risk on the next weld too?

It fixes that stop, not the condition. If heat input right before the stop was already thin, the next stop carries the same risk regardless of technique at the crater.

## See the condition, not the consequence

Most weld imperfections are produced by conditions that exist while the arc is running. Therness records those conditions on every weld, so a suspect run is known on the shift that made it rather than in a batch report.