Discover HeatCore AI

ISO 6520-1 group 4 · Lack of fusion and penetration

Lack of inter-run fusion (ISO 6520-1 ref. 4012): causes and detection

ISO 6520-1 reference 4012 is a planar imperfection between passes in a multi-pass weld, distinct from sidewall and root fusion failures. Cause matrix, the geometry test that locates it, and where acceptance is set.

ISO 6520-1 reference
4012
Group
4 — Lack of fusion and penetration
Also called
Lack of inter-run fusion, Interpass lack of fusion

Reference 4012 narrows reference 401 to a specific location inside a multi-pass weld: not the bevel face, not the root, but the boundary between two stacked passes. What decides it is the previous bead’s condition at that boundary — profile, cleanliness and placement — not just the new pass’s energy.

The cause matrix mirrors that: slag or oxide left on the previous pass blocks bonding outright; a previous bead too convex or placed off centre leaves a toe crevice the next pass can bridge without remelting into it; and arc energy too low on the new pass fails to remelt the previous bead across its full width.

Detection follows the family pattern — visual inspection cannot see a buried interface, ultrasonic and phased array testing lead because the imperfection is planar — but the pool camera view is more specific here than for the other two sub-types: it can watch the new pass actually wet the previous bead’s toes, the geometry this designation turns on.

See reference 401, lack of fusion, in general; reference 4011, lack of sidewall fusion; and reference 4013, lack of root fusion, the other two locations.

Typical causes

What produces lack of inter-run fusion, the mechanism, and the control that removes it
CauseMechanismControl
Slag or oxide left on the previous passA residue film across the top of a completed pass blocks bonding even when the new pass's thermal conditions are correct.Enforce interpass cleaning as a hold point between every pass and record that it happened.
Previous bead too convex, or placed off the joint centrelineAn over-convex bead, or one off the groove centre, leaves a toe crevice the next pass can bridge without remelting into it.Check bead profile and toe placement against the WPS between passes, not only cap width and reinforcement height.
Arc energy on the new pass insufficient to remelt the previous beadLow current, high travel speed, or a short arc all reduce the chance that remelting reaches the full width of the previous bead.Compute arc energy from measured current, voltage and travel speed per pass, not a procedure-wide setting.

Detection: which route finds it

The column that matters most is the last one. An inspection family marked as not finding this imperfection will not find it however carefully it is applied, and planning around that is cheaper than discovering it during a final examination.

Detection routes for lack of inter-run fusion, and what each one can and cannot see
FamilyMethodCapabilityWhat it sees
VisualVisual testing to ISO 17637Does not find itThe interface between two passes is buried the moment the next pass covers it.
ThermalIn-process infrared thermographySupporting signalSees the conditions that produce it — a cold toe crevice or insufficient remelt energy — rather than the buried interface itself.
CameraHigh-speed weld pool imagingSupporting signalShows whether the new pass's pool wets into the previous bead's surface across its full width, including at the toes.
NDTUltrasonic and phased array testing to ISO 17640 and ISO 13588Primary routeThe leading route for a planar imperfection at an interpass boundary. Radiography can miss one when the plane is unfavourable to the beam.

Where acceptance is defined

Therness pages never reproduce a standard's acceptance values: those tables are copyrighted and belong in the copy you hold. What follows is the pointer — which document governs, and which part of it to open.

Documents that set the acceptance criteria, and the clause topic to read
StandardClause topicNote
ISO 5817Quality levels for planar imperfections, indexed by ISO 6520-1 reference numberTreated under the same strict planar-imperfection rows as the parent reference 401.
ISO 11666Ultrasonic acceptance levels for welds, paired with the quality level chosenThe examination standard and the quality-level standard are selected together.

Questions about lack of inter-run fusion

How is lack of inter-run fusion different from sidewall or root lack of fusion?

All three are ISO 6520-1 group 401, and all three are the same bonding failure. The difference is location: 4011 sits at the bevel face, 4013 sits at the root, and 4012 sits between two weld passes inside the multi-pass fill.

What condition is most specific to reference 4012 among the three lack-of-fusion sub-types?

Bead profile and placement of the previous pass: an over-convex or off-centre bead leaves a toe crevice the next pass can bridge without remelting into it — a geometry specific to this boundary.

Can radiography reliably find lack of inter-run fusion?

Not reliably. Like sidewall and root lack of fusion, it is planar, and radiography's sensitivity depends on the angle between the defect plane and the beam. Ultrasonic and phased array testing lead because they do not share that limitation.

See the condition, not the consequence

Most weld imperfections are produced by conditions that exist while the arc is running. Therness records those conditions on every weld, so a suspect run is known on the shift that made it rather than in a batch report.

Progetto cofinanziato nell'ambito del PR Piemonte FSE+ 2021-2027,
Priorità I, Obiettivo Specifico a), Azione 4 – "Sostegno alla nascita delle start up"