Railway rolling stock manufacturing
Railway weld monitoring for EN 15085 rolling stock
Thermal and process records for every weld on car bodies, underframes and bogies: what they show, how a one-cell pilot runs and what goes into the EN 15085 file.
ISO 6520-1 group 6 · Miscellaneous imperfections
ISO 6520-1 reference 601 covers arc strike, accidental arc initiation on parent material outside the joint. Cause matrix, why the surrounding surface needs its own sweep, and the standards treating it as a defect.
An arc strike happens away from the joint being welded: a stray electrode touch, a ground clamp arcing at a poor contact, or a torch rested live on the workpiece for an instant. The energy is small next to a production weld, but it melts a spot of parent material and lets it re-solidify with no filler, shielding or control over the result — closer to an uncontrolled miniature weld than to a scratch.
On steels susceptible to hardening, that uncontrolled cycle is the concern: a fast self-quench can leave a small hard, brittle spot right where the notch the strike leaves behind concentrates stress. ISO 5817 treats an arc strike as a defect in its own right, independent of the weld’s own quality.
Because the mark sits on parent material, it is found by sweeping the surrounding surface during visual inspection, not only the seam — a step easy to skip. A ground-out strike on a critical structure is typically verified afterward with the same route that would find a crack, since removing discoloration does not confirm the affected, possibly hardened material is gone. Spatter from the same stray contact is common and worth checking at the same time.
| Cause | Mechanism | Control |
|---|---|---|
| Stray or dropped electrode contact outside the joint | A momentary, uncontrolled arc melts a small volume of parent material away from the weld and lets it re-solidify with no shielding or filler. | Enforce electrode handling procedures at fit-up and tack stages, where most strikes occur. |
| Poor ground clamp connection | A loose or corroded clamp arcs at its own contact point on the workpiece whenever current tries to find a path through it. | Inspect and maintain ground connections as a routine equipment check, not only after a strike is found. |
| Torch or electrode rested live on the workpiece | Even a momentary contact outside the joint delivers the same fast heat-and-quench cycle as a deliberate strike. | Train and enforce a dead-torch rule between passes and at breaks, particularly on hardenable steels. |
The column that matters most is the last one. An inspection family marked as not finding this imperfection will not find it however carefully it is applied, and planning around that is cheaper than discovering it during a final examination.
| Family | Method | Capability | What it sees |
|---|---|---|---|
| Visual | Visual testing to ISO 17637, sweeping the parent surface beyond the joint | Primary route | The mark is directly visible on bare metal once an inspector looks at the surrounding surface, not only the seam itself. |
| Thermal | In-process infrared thermography | Limited | A brief heating event away from the weld path can register as a transient, but a system tuned to the joint is not aimed there. |
| Camera | High-speed weld pool imaging | Does not find it | The camera is aimed at the weld pool in the joint; a stray arc away from that field of view is outside what it observes. |
| NDT | Magnetic particle or penetrant testing to ISO 17638 and ISO 3452-1 | Primary route | Verifies that a ground-out strike, and any resulting crack in a hardened spot, has actually been removed rather than only cosmetically dressed. |
Therness pages never reproduce a standard's acceptance values: those tables are copyrighted and belong in the copy you hold. What follows is the pointer — which document governs, and which part of it to open.
| Standard | Clause topic | Note |
|---|---|---|
| ISO 5817 | Acceptance of arc strikes as a defect condition in their own right, indexed by ISO 6520-1 reference number | Treated independent of the weld's own quality; the parent material outside the joint is in scope too. |
| AWS D1.1 | Workmanship requirements prohibiting arc strikes on structural steel outside the weld joint | Structural codes commonly require removal and verification rather than acceptance at any size on critical members. |
No. It is a fast, uncontrolled heating and quenching cycle on unprepared parent metal, which on hardenable steels can leave a small hard, crack-susceptible spot under a mark that looks superficial.
Grinding removes visible discoloration but does not confirm the affected material and any crack are gone; a critical structure typically verifies the ground-out area with the same route that would find a crack.
Beyond the seam — on the parent material surrounding the joint, where a stray electrode or ground-clamp contact actually happens. Attention fixed only on the weld itself misses them.
Most weld imperfections are produced by conditions that exist while the arc is running. Therness records those conditions on every weld, so a suspect run is known on the shift that made it rather than in a batch report.