Discover HeatCore AI

ISO 6520-1 group 6 · Miscellaneous imperfections

Spatter (ISO 6520-1 ref. 602): causes and detection

ISO 6520-1 reference 602 covers spatter, molten metal ejected from the arc that lands outside the weld. Cause matrix, why a rising rate signals arc instability, and the standards treating it as a surface condition.

ISO 6520-1 reference
602
Group
6 — Miscellaneous imperfections
Also called
Spatter, Weld spatter

Spatter is metal that leaves the process without becoming weld: droplets ejected from the arc or the pool that land on the surrounding parent material instead of joining the joint. In short-circuit transfer the wire bridges to the pool and the current surge can eject droplets before a clean transfer occurs; in globular transfer, oversized drops detach irregularly under gravity. Both routes are sensitive to arc voltage, inductance and shielding gas, so a change in any of them shows up as a change in spatter rate before anywhere else.

That sensitivity is why spatter earns more attention than its cosmetic reputation suggests. A weld can be structurally sound and still throw spatter, but a rising rate during an otherwise unchanged run is an early symptom of the same arc instability that, left uncorrected, goes on to disturb pool geometry and raise the risk of porosity and inconsistent fusion.

Adherent spatter fused onto the finished surface is a distinct condition from loose spatter that brushes off, because adherent particles can sit close enough to the joint to interfere with later NDT or coating adhesion. It shares a location with arc strikes — both put unwanted metal or heat outside the intended weld path — though the mechanisms differ.

Typical causes

What produces spatter, the mechanism, and the control that removes it
CauseMechanismControl
Short-circuit transfer instability in GMAWThe wire bridges to the pool, the circuit shorts, and an uncontrolled current surge can vaporise the bridge violently enough to eject droplets before a clean transfer occurs.Tune arc voltage and inductance to the window qualified for the wire and gas, not a generic panel setting.
Globular transfer from excess arc length or currentOversized drops detach irregularly under gravity instead of at a controlled rate, throwing metal outside the joint.Keep current and arc voltage inside the range qualified for spray or controlled short-circuit transfer for the material and position.
Shielding gas composition or flow drifting out of specificationA shift in gas mix or coverage changes arc behaviour before it changes anything else visible in the weld.Monitor gas flow and composition continuously; a rising spatter rate is often the first symptom of a drifting gas supply.

Detection: which route finds it

The column that matters most is the last one. An inspection family marked as not finding this imperfection will not find it however carefully it is applied, and planning around that is cheaper than discovering it during a final examination.

Detection routes for spatter, and what each one can and cannot see
FamilyMethodCapabilityWhat it sees
VisualVisual testing to ISO 17637, of the parent surface around the weldPrimary routeAdherent spatter on the finished surface is directly visible and distinguished from loose spatter during the same inspection.
ThermalIn-process infrared thermographyLimitedIndividual spatter droplets are too brief and small to register reliably against the weld pool's own thermal signature.
CameraHigh-speed weld pool imagingPrimary routeDirectly counts and times ejected droplets, which is why a rising spatter rate is read as an arc-instability signal before anything else changes.
NDTRadiographic or ultrasonic testing to ISO 17636 or ISO 17640Does not find itSpatter sits on the surface outside the weld; volumetric methods aimed into the joint do not examine it at all.

Where acceptance is defined

Therness pages never reproduce a standard's acceptance values: those tables are copyrighted and belong in the copy you hold. What follows is the pointer — which document governs, and which part of it to open.

Documents that set the acceptance criteria, and the clause topic to read
StandardClause topicNote
ISO 5817Acceptance of spatter, indexed by ISO 6520-1 reference numberAssessed as a surface condition on the finished part, separate from any internal soundness criterion for the weld itself.
AWS D1.1Workmanship requirements for removal of spatter adherent to the finished structural surfaceStructural codes commonly require removal before coating or further fabrication rather than setting a size limit.

Questions about spatter

Does spatter mean the weld itself is defective?

Not necessarily. A sound weld can still throw spatter; the reason to watch it is that a rising rate during an otherwise unchanged run is an early sign of the arc instability that goes on to disturb pool geometry and fusion.

Is loose spatter treated the same as adherent spatter?

No. Loose spatter brushes off; adherent spatter fuses onto the surface and can interfere with later NDT or coating adhesion, so specifications commonly treat the two separately.

Which welding process produces the most spatter?

Gas metal arc welding in short-circuit or globular transfer produces the most, because both mechanisms eject droplets as a normal part of how the arc transfers metal, unlike spray transfer.

See the condition, not the consequence

Most weld imperfections are produced by conditions that exist while the arc is running. Therness records those conditions on every weld, so a suspect run is known on the shift that made it rather than in a batch report.

Progetto cofinanziato nell'ambito del PR Piemonte FSE+ 2021-2027,