A preheat temperature on a WPS looks like a single fact: 100 °C, say, minimum. Behind it sits a calculation with four inputs, two possible methods and at least one trade-off that a production change can quietly undo. EN 1011-2 is where that calculation lives for arc welding of ferritic steels. Whether the standard applies to your joint at all is a separate question, answered on the EN 1011-2 standard page. This article starts after that decision: you know it applies, and you need to work out what the minimum preheat is, why, and how to show the joint actually got there.
Key takeaways
- EN 1011-2 sets a minimum preheat to keep a ferritic steel joint out of hydrogen (cold) cracking, from four inputs: composition, thickness, hydrogen and heat input.
- Annex C gives two routes. Method A reads diagrams keyed on CEV, combined thickness, a hydrogen scale and heat input. Method B is an equation in CET, plate thickness, diffusible hydrogen and heat input.
- The two methods use different carbon equivalents and different thickness definitions. Feeding one method’s inputs into the other is the most common arithmetic error.
- Composition, thickness and hydrogen push the preheat up; heat input pulls it down, within the range the method covers.
- The result is a floor for the whole weld, not a temperature to reach once before the first run.
- A preheat that was never measured to ISO 13916 is a number on paper. The record is what turns it into a control.
What the number is protecting against
Hydrogen cracking needs three things at once: a hard, crack-sensitive microstructure in the heat-affected zone or weld metal, diffusible hydrogen dissolved in it, and tensile stress. Remove any one and the crack does not form. Preheat works on the first two together. It slows the cooling of the joint, so the heat-affected zone transforms to a softer microstructure, and it keeps the joint warm long enough for part of the hydrogen to diffuse out before the steel reaches the temperature range where it gets trapped.
That is why the calculation needs all four inputs. Composition decides how readily the steel hardens. Thickness decides how fast the joint is cooled by the surrounding metal. Hydrogen decides how much is available to cause trouble. Heat input decides how much heat the arc itself puts in. None of them alone tells you the preheat, and a change to any one of them on the shop floor changes the answer.
The cracks are also slow. Hydrogen cracking can appear hours after the weld is finished, which is why some specifications hold inspection back for a period after welding. The hold time before inspection is the downstream half of the same problem; preheat is the upstream half.
The four inputs, and where each comes from
Composition. The mill certificate gives the weight percent of carbon and the alloying elements. Both methods compress it into a single carbon equivalent, but not the same one: Method A uses the IIW carbon equivalent CEV, Method B uses CET. They weight the elements differently and they are not interchangeable. A CEV of 0.40 and a CET of 0.40 describe very different steels. The carbon equivalent glossary entry explains what the index represents, and the carbon equivalent calculator returns both from one certificate.
Thickness. Here the methods differ in definition, not only in weighting. Method A works on combined thickness: the sum of the thicknesses of all the parts meeting at the joint, measured a defined distance away from the joint line. Method B works on plate thickness, and where the plates differ the thicker one governs. More on why that matters below.
Hydrogen. The diffusible hydrogen content of the weld metal is measured to ISO 3690 and given on the consumable datasheet in ml per 100 g of deposited metal. Method B takes that number directly. Method A groups it into hydrogen scale letters, each covering a band defined in the standard; you find which band your consumable and process fall into and use that letter.
Heat input. The heat input of the run in kJ/mm, taken from the WPS. It has to be heat input, not arc energy: if the WPS quotes arc energy, apply the process thermal efficiency factor first. The heat input calculator does the conversion, and the heat input guide explains which convention each standard means.
Method A: the diagrams
Method A gives a set of diagrams. Each diagram corresponds to a band of carbon equivalent and a hydrogen scale; on it, the minimum preheat is read from the intersection of combined thickness and heat input. The procedure is mechanical once the inputs are right:
- Work out CEV from the mill certificate.
- Find the hydrogen scale letter that the consumable and process fall into.
- Pick the diagram for that CEV band and hydrogen scale.
- Work out the combined thickness of the joint.
- Read the minimum preheat at the intersection of combined thickness and heat input.
The diagrams are part of the standard and are not reproduced here. The preheat temperature calculator computes CEV and the combined thickness for you and records the hydrogen scale you are working to, so the values you take to the diagram are documented, but the reading itself is done in your copy of EN 1011-2.
Combined thickness, and why it is not the plate thickness
Combined thickness describes how many paths the heat has to escape the joint. A butt weld between two plates has two paths. A T-joint has three: the web and the flange on each side of it. A T-joint made of three 20 mm members therefore behaves, thermally, like a much heavier section than any of its parts, and its cooling is correspondingly faster.
For the combined thickness, the standard defines where each part is measured, which matters on tapered or machined parts where the thickness at the joint is not the nominal plate thickness. Take the dimension from the drawing at that location, not from the material order.
Method B: the equation
Method B replaces the diagrams with one expression. In the form published in Annex C as equation C.8, with CET from equation C.2:
- CET [%] = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40
- Tp [°C] = 697 × CET + 160 × tanh(d/35) + 62 × HD0.35 + (53 × CET − 32) × Q − 328
where d is the plate thickness in mm, HD the diffusible hydrogen in ml/100 g and Q the heat input in kJ/mm. Each term maps to one of the four inputs, which makes the equation easy to read once you look at it term by term:
- 697 × CET — composition. The steeper the carbon equivalent, the higher the preheat, roughly in proportion.
- 160 × tanh(d/35) — thickness. The hyperbolic tangent rises quickly at first and then flattens: going from 10 to 30 mm moves the answer a lot, going from 60 to 90 mm moves it much less, because beyond a certain section the joint is already cooled as fast as it will be.
- 62 × HD0.35 — hydrogen. The fractional exponent means the first few ml/100 g count most. Moving from a high-hydrogen to a low-hydrogen consumable moves the answer by tens of degrees.
- (53 × CET − 32) × Q — heat input. For any CET below about 0.60, the bracket is negative, so more heat input lowers the preheat.
The equation has a stated range of validity: CET from 0.20 to 0.50 %, plate thickness 10 to 90 mm, hydrogen 1 to 20 ml/100 g, heat input 0.5 to 4.0 kJ/mm, and parent metal yield strength up to 1000 N/mm². Inside that range the arithmetic is the method. Outside it, the formula still returns a number, and the number stops meaning what it says.
Do not mix the inputs. Method B uses CET and plate thickness. Feeding it CEV, or a combined thickness, produces a confident and wrong answer. The thickness case is the common one: the tanh term is already close to its ceiling at large thickness, so a combined thickness of a T-joint inflates the result without telling you anything about the joint.
A worked example, and what moves the answer
Take an illustrative carbon-manganese steel with a certificate reading C 0.16, Mn 1.40, Mo 0.02, Cr 0.10, Cu 0.20, Ni 0.15 (wt %). CET works out at about 0.32. Weld a 25 mm plate with a consumable at 5 ml/100 g and a heat input of 1.2 kJ/mm, and Method B returns a minimum preheat of about 85 °C. This is an illustration of the published equation, not a recommendation for any real steel or joint: the WPS and the material specification govern.
Now change one input at a time and keep the rest:
- Hydrogen to 2 ml/100 g: the answer falls to about 55 °C. To 10 ml/100 g, it rises to about 115 °C. The consumable and its storage are worth around 60 °C of preheat on this joint.
- Heat input to 2.0 kJ/mm: the answer falls to about 73 °C. To 0.8 kJ/mm, it rises to about 91 °C. The effect is real but smaller than hydrogen on this steel.
- Thickness to 40 mm: about 117 °C. To 60 mm: about 136 °C. To 90 mm: about 145 °C. The curve flattens as the section grows.
- CET to 0.40: about 145 °C. Every 0.05 of CET is worth roughly 38 °C here.
Two practical readings follow from those numbers. First, the hydrogen input is the one most likely to drift without anyone changing the WPS: an electrode left out of its oven, a flux-cored wire from a different production run, a damp shift. Second, the heat-input trade is the one most likely to be used on purpose. A welder who runs hotter to save preheat is following the arithmetic, but a longer cooling time affects the heat-affected zone in the other direction, and the t8/5 cooling time has to stay inside the window the procedure qualified.
Choosing between the two methods
Both methods aim at the same outcome, and EN 1011-2 presents them side by side. They are built on different data and different input definitions, so the same joint will not necessarily return the same temperature from both. A few practical points decide which one a fabricator uses:
- Range of application. Each method states the steels and conditions it is meant for. Method B’s numeric range is listed above; check the scope paragraph of Method A in the standard before relying on its diagrams for a higher-strength or more highly alloyed steel.
- What the certificate gives you. CET needs carbon, manganese, molybdenum, chromium, copper and nickel. CEV adds vanadium. A certificate that does not report an element you need is a gap to close with the supplier, not a zero to assume.
- What the WPS and the contract already say. EN 1011-2 is a recommendations document. If the qualified WPS or the contract fixes a preheat, that number governs, and the method is the reasoning behind it.
- Consistency. Whichever method a procedure was built on, keep using it when you re-check that procedure. Switching method between the WPS and a production query produces two numbers and an argument.
What neither method sees is just as important. The calculation does not know how restrained the joint is, how well it was fitted, whether there is moisture or frost on the preparation, or whether the shop floor is at 5 °C on a winter morning. A result at or below ambient means the calculation finds no hydrogen-cracking need for preheat on those inputs. It does not mean the joint can be welded cold and wet.
From a number on the WPS to a temperature at the joint
The result of either method is a minimum. It applies from the first run to the last, and it is also the floor below which the joint should not drop between runs. On a multi-run weld the dangerous moment is rarely the first pass, which everyone checks. It is the pass after a break, a shift change or a repair, when the plate has cooled back below the minimum and the welder resumes without measuring again. That is the failure mode behind much hydrogen-induced cracking.
ISO 13916 defines how the temperature is measured: at a distance from the edge of the joint preparation that depends on the thickness, on the face opposite the heat source where that is possible, and after a waiting time that also grows with thickness so the heat has soaked through. The guide to preheat and interpass monitoring to ISO 13916 walks through the measurement positions and the evidence an auditor expects.
A temperature-indicating crayon or a contact probe answers the question at one point and one moment. It cannot say whether the far end of a two-metre seam was at temperature, or whether the joint stayed above the minimum through the fourth pass. A thermal camera looking at the joint records the surface temperature across the whole area and for every pass, so the preheat and interpass minimum in the WPS can be checked against what actually happened, joint by joint.
Keep the calculation with the record. The inputs used for the preheat — certificate, thickness, hydrogen level, heat input and the method chosen — belong in the job file next to the measured temperatures. When a crack turns up, the first question is whether the joint was below the minimum or whether the minimum was wrong, and only the two records together answer it.
What to keep on file per joint
- The method used (A or B) and the edition of EN 1011-2 the WPS was derived from.
- The carbon equivalent and the certificate it was calculated from.
- The thickness used, and whether it was combined thickness (Method A) or plate thickness (Method B).
- The consumable, its hydrogen level and how it was stored and handed out.
- The heat input range of the WPS and the heat input actually run.
- The measured preheat and interpass temperatures, with position, time and pass, taken to ISO 13916.
With those six items, a preheat is a traceable decision. Without them, it is a value someone wrote on a form.
Related reading
- EN 1011-2: does it govern your preheat and cracking risk
- Preheat temperature calculator (EN 1011-2, CET)
- Preheat and interpass temperature monitoring to ISO 13916
- Carbon equivalent: definition, formula and use
- Preheat temperature: definition
- Interpass temperature: definition
- Delayed hydrogen cracking: inspection hold time after welding
- Measuring weld cooling rate and t8/5 with thermography
A preheat number is a claim until something records it
HeatCam thermal cameras watch the joint and log the surface temperature for every pass, so the preheat and interpass minimum in the WPS becomes a timestamped record across the whole joint instead of a crayon mark someone remembers making.
Request a HeatCam demoTherness solution: Welding camera — Thermal and high-speed imaging that watches the arc, the pool and the cooling seam while the weld is made.
Frequently Asked Questions
What is the difference between Method A and Method B in EN 1011-2?
Both sit in Annex C and both aim at the same thing: a minimum preheat that keeps a ferritic steel joint out of hydrogen cracking. Method A reads the temperature off a family of diagrams keyed on the IIW carbon equivalent (CEV), the combined thickness of the joint, a hydrogen scale letter and the heat input. Method B is an equation that takes the CET carbon equivalent, the plate thickness, the diffusible hydrogen content in ml/100 g and the heat input, and returns a temperature directly.
Which inputs do I need to calculate preheat to EN 1011-2?
Four: the parent metal composition from the mill certificate (turned into a carbon equivalent), the thickness at the joint, the hydrogen level of the consumable and process, and the heat input of the run. Each method expresses them slightly differently: Method A wants CEV, combined thickness and a hydrogen scale letter; Method B wants CET, plate thickness and the hydrogen content as a number.
Does higher heat input reduce the required preheat?
Within the range the method covers, yes. A larger heat input slows the cooling of the joint on its own, so less external heat is needed to reach the same cooling time. In the Method B equation the heat-input term carries a negative coefficient for any CET below about 0.60. It is a trade, not a free reduction: more heat input lengthens the cooling time and can move the heat-affected zone out of its toughness window.
Is the EN 1011-2 preheat also the minimum interpass temperature?
The calculated temperature is a floor for the whole weld, not an event at the start: it is the temperature the joint should not fall below between runs. On a multi-run joint the risk sits in the pass welded after a break, when the plate has cooled below the minimum and nobody measured it again.
How do I prove that the preheat was actually reached?
By measuring it the way ISO 13916 describes: at a defined distance from the joint preparation that depends on thickness, on the face opposite the heat source where possible, and after a waiting time that also grows with thickness. A reading at one point and one moment proves that point and that moment; a record across the joint and across every pass proves the weld.
Is EN 1011-2 mandatory?
It is a recommendations document. A qualified WPS or a contract that already fixes a preheat and interpass regime takes precedence, and the standard is the method behind that number rather than an override of it. Whether EN 1011-2 governs your case at all is a scope question covered on the standard page.